Features and applications
Product characteristics
- Excellent welding operation properties including smooth and fine ripple weld surface and easy slag removal.
- Designed for pairing with GLES-95 weld on high manganese austen ti tic steels to achieve higher than 80 o MPa tensile strength.
- Low levels of residue elements deliver good results on -196°C impact.
Applications
- LNG cryogenic storage tank
- Pressure vessel
- Weld on high manganese austen ti tic steels
Standards
- EN ISO 14174 SAFB2AC
Main Constituents (%)
Values in percent by mass.
| SiO₂ + TiO₂ | MnO + Al₂O₃ | CaO + MgO | CaF₂ |
|---|---|---|---|
| 15 | 20 | 40 | 25 |
Mechanical Properties of All Weld Metal
Typical all-weld-metal mechanical properties.
| WIRE | PWHT | Yield Strength (MPa) | Tensile Strength (MPa) | Elongation (%) | Charpy test temperature (°C) | Charpy impact energy (J) |
|---|---|---|---|---|---|---|
| GLES-95 | AW | 430 | 810 | 50 | -196 | 75 |
Typical Analysis of All Weld Metal (%)
Values in percent by mass.
| WIRE | C | Mn | Si | Cr | S |
|---|---|---|---|---|---|
| GLES-95 | 0.50 | 25.0 | 0.32 | 3.1 | 0.005 |
Notes
- 1. Damp flux should be redried at 300-350°C for 2 hours.
- 2. Mill scale, rust, oil and slag must be removed from the base metal.
- 3. At least 20% new flux must be added into recycled flux.